TECHNICAL SUPPORT

Frequently asked questions

The questions engineers and buyers ask us most about kiln furniture and ceramic fiber insulation. If yours is not here, send it to us: it is answered by our technical team.

Setter plates

Go to the page

The datasheet says 1700 °C. Why did my plate warp at a lower temperature?

The maximum service temperature describes the material at near-zero load. The heavier the product on the plate, the lower the temperature at which it bends. Tell us both the temperature and the load when you choose a plate.

Why do setter plates crack, and do expansion slots help?

Cracking depends on cooling rate, load, plate size, stacking height and process. Expansion slots relieve stress but cannot guarantee a crack-free plate. Before full production, run a small batch on your line.

Why does product stick to the plate? Will grinding fix it?

Sticking is usually a reaction between the plate material and the product, so it comes back after grinding. Change the material, or add a barrier layer such as a zirconia coating.

What flatness can you hold?

Flatness depends on size, thickness and grade, so there is no single figure. Send us the size and your requirement, and we confirm it for that grade.

Porous setters and 99DK

Go to the page

Porous setter or the high-porosity 99DK plate?

99DK gives the best debinding and is our first recommendation; if the lattice pattern on your product is a concern, choose 99DK. In practice, use whichever works in your process. If both work, choose the more cost-effective one. Note that 99DK cannot carry load.

The lattice pattern shows on my product. What can I do?

The mark is the shape of the plate surface, not a reaction between plate and product. If the product is ground after firing, it does not matter. For sensitive surfaces, switch to G5-1 and place the product on the flat face.

I switched to porous setters and my products started cracking. Why?

Porous setters let the binder out faster and more completely, so your old heating curve is now too fast and corners crack. Lower the heating rate after switching.

What is the highest temperature I can use?

The material is rated to 1550 °C at near-zero load. How hot you can actually go depends on the weight on the plate: the heavier the product, the more easily the plate deforms, and a very heavy product can bend a plate even at 1000 °C. Tell us your temperature and load, and we suggest a thickness or a dense setter instead.

Can you make larger plates?

Yes. We ask you to trial with the standard 150 × 150 × 2 mm size first, so each test does not need a new size. Once the trial passes, we discuss the size you need for production.

MLCC setter racks and nickel mesh

Go to the page

Why do setter racks break?

Three common causes: the long-term temperature is too high (keep it below about 1400 °C); the rack is supported differently in use than when it was fired, so stress concentrates; or it is lifted by one corner. If racks still break, send us your kiln type, loading and photos of the break.

Why does the zirconia coating come off the mesh?

Usual causes are oxygen in the atmosphere, an uneven coating, or poor adhesion. Use the mesh only in a reducing or inert atmosphere.

Why does the mesh warp?

Most often because it is supported only at the edges. Lay the mesh on a rack so it is supported across its area.

Can the mesh be used in air?

We advise against it. In air, nickel oxidizes and expands, which pushes the zirconia coating off.

The sample passed. Why did the defect rate rise in volume production?

In a full kiln the middle and the edges heat unevenly, and loading, kiln type and raw material lots also play a part. Start with a small batch and adjust the curve for production.

Pusher plates and kiln posts

Go to the page

Why do our pusher plates crack?

Most often because of fast heating or cooling. Slow down the push rate and the cooling, and check that the long-term temperature stays near 1400 °C. If cracks continue, send us the kiln type, push rate, load and photos.

Can we use other setter grades as pusher plates?

We do not recommend it. Only 86C-3 performs well as a pusher plate in our range.

Can you make posts to our size?

Yes. Send us a drawing or the dimensions and the load they carry. The nine sizes listed on the product page have been made before and can be made again.

ITO target setters

Go to the page

Why use a separate setter under the target?

The setter plate below is chosen for strength and flatness at large size. The high-purity setter on top is chosen for purity, because it is the part that touches the target.

Can you make setters to our target size?

Yes. Our standard disc is Ø35 × 10 mm; square plates and other sizes are made to your drawing, with both faces ground. The large setter plate below is also made to your requirements.

LTCC and HTCC

Go to the page

Our substrates warp or come out dark. Is it the setter?

Not always. Warping and darkening often start earlier in the process: tape, paste, lamination or the burnout profile. The setter can play a part, through flatness, permeability or the way the stack is supported. Send us your conditions and photos, and we check together whether the kiln furniture is part of the cause.

Which setter should we start with?

For LTCC debinding and sintering, 1300HS or a permeable plate such as 99DK. For HTCC, 99-Z1 or porous setters. Tell us your paste, temperatures and substrate size, and we suggest a starting point and a sample.

Ceramic fiber blankets and boards

Go to the page

Board or blanket?

Boards are rigid, machinable and keep their shape, which suits chamber walls and parts that face the flame. Blankets are flexible and fit curved shapes, seals and modules. Many linings use both.

Which grade do I need?

Start from the continuous temperature where the blanket sits. On the hot face you may need a higher grade than behind it. Tell us your furnace and lining, and we suggest a combination.

Which density should I choose?

Higher density gives more strength and is often used on the hot face; lower density is lighter and cheaper for backing and wrapping. Tell us where it goes and we suggest one.

Is the MAFTEC™ 1600-grade blanket a 1600 °C blanket?

No. "1600" is the grade name. The blanket is used long-term at 1500 °C on the hot face; full 1600-grade modules are used long-term at 1500–1600 °C.

Hot face or backing?

The 1600-grade blanket is meant for the hot face. Behind it, a more economical blanket is usually enough. Tell us your lining and we suggest a combination.

Can you supply boards cut to shape?

Yes. Boards can be cut and machined to your drawing.

Can you supply modules?

Yes. Blankets can be folded into modules, including combinations of a high grade on the hot face with a lower grade behind it.

Working with us

Go to the page

Are you a manufacturer?

No. YOUKA TECH is a trading company in Suzhou, China. Our products are made by long-term manufacturing partners. Factory audits are welcome; we arrange and accompany the visit.

Can I test a sample first?

Yes. Most products can be sampled so you can test them in your own kiln. Tell us the product and size.

Are the values on this site guaranteed?

They are typical values (averages), not guaranteed values. Specification values are agreed in the technical agreement.

What should I include in my inquiry?

For a price: the product, size and quantity. For a recommendation: what you fire, the maximum temperature, the atmosphere, the kiln or furnace type and the problem you see. Drawings and photos help.

What happens after I send an inquiry?

We usually reply within 1–3 business days. If a technical question needs more time, we first send a short reply and tell you when to expect the full answer. Then: we confirm the details and recommend a product, send a sample if you want to test it, start with a small batch, and move to regular orders.

How do I place an order?

Send us an inquiry with the product, size and quantity. Orders can be placed through our Alibaba.com store.

Have a question that is not here?

Send it with your conditions and, if you can, photos. Our technical team usually replies within 1–3 business days; for complex questions we first send a short reply.

Ask a question